Abstract
Keywords
[Research]
Fabrication of UV/ TiO2 nanotubes / Pd system by electrochemical anodization for furfural photocatalytic degradation
H. Dehghani Ashkezari 1, H. Sid kalal 2*, H. Hoveidi 3, M.R.Almasian 2, M. Ashoor 4
1- University of Tehran Aras international campus, Aras, Iran.
2- Materials and Nuclear Fuel Research School, Nuclear Science and Technology Research Institute, AEOI, P.O. Box 11365-3486, Tehran, Iran.
3- Graduate Faculty of Environment, University of Tehran, Tehran, Iran
4- Radiation Application Research School, Nuclear Science and Technology Research Institute, Atomic Energy Organization of Iran, Tehran, Iran.
* Corresponding author’s E-mail: hsidkalal@aeoi.org.ir
(Received: Sept. 08. 2016 Accepted: Feb. 05. 2017)
ABSTRACT
The aim of this study was to degrade furfural by a new nanotube system. To degrade some organic pollutants as well as to reduce the amount of furfural which is a well-known pollutant in oil industry, the photocatalytic process along with ultraviolet (UV) irradiation may be employed. In this study, the UV/TiO2/Pd system in which the nanoparticles of palladium doped into the titanium dioxide was proposed for degradation of furfural. The rate of furfural decomposition in the proposed system was more than that of the system without TiO2 foils due to the degradable reactions. The experimental results demonstrate that the maximum degradation occurs at a distinct pH and specific temperature under the UV irradiation. After 100-minute UV-irradiation duration, the maximum and minimum degradations were 97.8% (pH 3), and 95.8% (pH 12), respectively. Also, the degradation values were as parabolic function at the pH values. The values of efficiency of decomposition for this irradiation duration at optimum pH 3 were 96.7% and 98.5% at 30◦C and 40◦C, respectively. Also, the minimum degradation under photolysis was 93.52% at 30oC under 20-minute UV-irradiation duration. Furthermore, while the irradiation duration was 70-75 min, the degradation values were independent of pH approximately. The difference between the degradation values at 30 and 40◦C was decreased with increasing the UV-irradiation duration till 60min, and then this difference was increased with increasing the UV-irradiation duration.
Key words: Furfural; UV/TiO2/Pd system; Photocatalytic degradation; Temperature; pH.
INTRODUCTION
The hydrology as well as the health may be affected by the pollution of environment. One of the pollution sources is the release of complex chemical materials from the various plants and facilities (Iliev et al. 2002). These materials are toxic and non-biodegradable in the biological systems which have a long life in natural environment because their decay and decomposition are insignificant. For instance, “Phenols” and “Furfural” are the cyclic and aromatic organic compounds that the latter is an aromatic aldehyde with the cyclic structure. As known, furfural is an excellent organic solvent to be employed to extract industrial effluents from other hydrocarbons and oil in the petrochemical and refineries which is consistent with the tissues and body organs due to high adsorption coefficient, as shown in Fig. 1. Recently, the oxidation techniques have been used to decompose the complex and heavy molecules. These oxidation reactions are included the Ultraviolet (UV) irradiation and/or a combination of other oxidizing agents and mineral catalysts (Wenqi et al. 2006; Faramarzpour et al. 2009; Borghei et al. 2008; Kang et al. 2009).Within the last few years, there are efforts to develop the some methods such as homogeneous and heterogeneous chemical oxidation, photo oxidation and photo catalysis in order to detoxify waste water efficiently. Also, the processes of silica-modified TiO2, titania-supported bimetallic catalyst, and TiO2/MgO are proposed as efficient ones to remove the various chemical complexes from waste water, and also as alternative for filtration, adsorption, reverse osmosis and incineration in environmental cleaning processes, dealing with complex nonbiodegradable chemicals (Boopathy et al. 1993; Nomeir et al. 1992; Haque 2007; He et al. 2013; Assadi et al. 2010; Huang et al. 2015; Chiou et al. 2008; Dixit et al. 2010; He et al. 2002; Ferrari-Lima et al. 2015; Kim et al. 2012; Sun et al. 2009).
In this study, a new method, combination of UV radiation and the nanoparticles of palladium were doped into the titanium dioxide (UV/TiO2/Pd) is proposed to degrade and to decompose the furfural in which the rate of furfural decomposition is more. The efficiency of various advanced oxidation processes (AOPs) and the effect of experimental parameters of pH, UV-irradiation duration, and temperature are also investigated on the rate of reactions.
Fig. 1. The structure of furfural.
MATERIALS AND METHODS
The titanium foils (1-mm thickness, 5×5 cm2, purity 99.5%), furfural (99.9%), palladium, platinum, stannous chloride II (SnCl2) and double distilled water were purchased from laboratory grade in Merck company. The technical specifications of furfural were as C2H4O2; molecular weight 96.09 g.mol-1; maximum UV-absorption wavelength 270 nm; boil point 11 Torre; density 1.159 mg.L-1 for standardization of pure analysis.
Experimental Procedures
Preparing TiO2 nanotube arrays by anodization process
As shown in Fig. 2, the titanium foils were anodized at three stages as follows; (a)
polishing with sand-paper, as shown in Fig. 3 A and B, (b) cleaning by the 100-ml solution consisting of HF (10 ml), HNO3 (40 ml), and (c) twice distilled water (50 ml) during 5 second and washing by distilled water.
These foils with the thickness 1mm, the surface area 25 cm2 and the purity 99.5% were ultrasonically cleaned in the detergent, acetone, ethanol, nitric acid, and deionized water in turn during 10 minutes, and then dried in an oven prior to the anodization process. For the anodic oxidation process, a two-electrode configuration was used with platinum foil as the counter electrode at a fixed potential, as shown in Fig. 4. The distance between two electrodes approximately was 3cm. The voltage value and duration of anodization were 60V and 120 min, respectively. The mixture of the HF (2 mL) and DMSO (98 mL) was used in different concentrations as electrolyte. The stirring rate was 150 rpm (Rui et al. 2011; Hee-Yeon et al. 2011; Yajun et al. 2011; Sreekantan et al. 2011; Robin et al. 2014; Hoyer 1996; Prakasam et al. 2007; Minagar et al. 2012; Regonini et al. 2013).
Samples were washed by deionized water and ultrasonicated to remove the ions from the surface of the TiO2 foils after anodization. All experiments were carried out at room temperature. The SEM images of TiO2 nanotubes /Pd were prepared by the scanning electron microscope, Zeiss evo 18, Germany, as shown in Fig. 5.
Gong et al. fabricated the TiO2 nanotube arrays by the anodic oxidation of titanium foil into the fluoride-electrolyte solution primarily that its mechanism is as follows (Gong et al. 2001);
The TiO2 passive layer is formed by the elemental titanium undergoing oxidation and hydrolysis in aqueous acidic medium (Macak et al. 2005) as:
Ti + 2H2O TiO2 + 4H
Fig. 2. Flowchart of implementation of the proposed method.
Fig. 3. Images of titanium foils before (A), and after anodization process (B).
Fig. 4. Two-electrode electrochemical cell for anodization process.
Fig. 5. SEM images of anodized TiO2 (A), and TiO2/Pd (B).
To form soluble [TiF6]-2 complexes, the TiO2 undergoes rapid etching in the presence of acidic HF or neutral fluoride containing solutions in spite of stability at the pH values from 2 to 12 thermodynamically. The Ti–O bond is weakened by the polarization so that the dissolution of metal oxide is increased at higher applied electric field.
This dissolution at higher voltage values leads to the field-assisted chemical dissolution of the oxide appeared at the oxide/electrolyte interface. The F_ ions are produced by the pits as follows,
TiO2+ 6HF [TiF6]-2 + 2H2O + 2H
Basically, the porous layer is dependent on the equilibrium between electrochemical formation and the chemical dissolution of TiO2
in solution of F _ ion. In this study, chemical composition of electrolyte was 2% HF in DMSO, and the nanoparticles were formed at duration of 12 h under the anodizing voltage 60V.
The localized dissolution of TiO2 and anodization of Ti in HF may occur simultaneously which the latter involves the electrochemical dissolution of titanium metal into Ti ions, the oxidation of Ti+ and/or Ti3+ to TiO2. After annealing the Ti foils at 450ºc for 2 h in oven, the TiO2 nanotubes (anatase) synthesis is completed (Rui et al. 2011).
Doping Pd
It was carried out at two synthetics stages. At first, TiO2 foils were dipped into the stannous chloride II (SnCl2) solution of 0.1M during two minutes before the ultrasonic process. At the second, the samples were settled in the PdCl2 solution of 0.01M during four minutes (Fig. 5A and B). The reactions were as follows,
Sn+2 → Sn+4 +2e and Pd+2 +2e →Pd Þ Pd+2+ Sn+2 → Pd + Sn+4
Experimental reactor consists mainly of a two-layer beaker with 1-litre capacity and a two-layer quartz mounting in the center of the photoreactor, as shown in Fig. 6. The heater was used to obtain a constantly suitable temperature in experiments. The cooling water system is used and injected to the annulus surrounding the beaker and lamp. To decrease errors and avoid noise, this reactor was placed in the cubic dark box at dimensions of 1m covered by the aluminum foil. The samples were drawn out from the reactor at the certain intervals for analysisby UV lamp (250W).
RESULTS AND DISCUSSION
The absorptiveness effect of titanium foil
To obtain the spectra of absorption, the system with/out titanium foil was irradiated by UV light during 100 minutes, as shown in Fig. 7.
The peak of 270 nm was considered as a criterion of the photocatalytic activity. The results show that the amount of absorption was increased in the presence of the titanium foil. After 100-minute UV-irradiation duration, the concentrations of the samples with/out titanium foil were 12.1 and 10.94 mg.L-1, respectively. To evaluate the photo degradation behavior of furfural in the UV/TiO2/Pd system, the second series of experiments were carried out in which the concentration of furfural was 250 mg.L-1 along with a medium pressure mercury lamp (250W) as the UV source. In the system without
titanium foil, the amount of absorption is decreased with increasing the wavelength value as exponential, while in the system with titanium foil, the minimum and maximum values are 1.22 and 1.38 at the 255nm and 270nm, respectively. Also, it decreased as exponential function approximately at more than 270nm.
The effect of various UV-irradiation durations
The photocatalytic test was done on the TiO2/Pd foils. The spectra were obtained during 100-minute UV irradiation, as shown in Fig. 8.
The photocatalytic activity was characterized by the peak intensity of 270 nm. The furfural has a configuration of absorption because there are the OH−ions on the surface of TiO2 foils. To more deliberation, the efficiency of degradation was defined as follows:
d = (Co − C)/Co × 100% [1]
Where Co and C are the concentrations of furfural before and after degradation, respectively.
The degradation of furfural took place up to 100-minute UV-irradiation duration in all the samples here. The efficiency of degradation severely increases with increasing duration of irradiation because of improving the photocatalytic activity of TiO2 (Pd).
To assess degradation of furfural, the first set of experiments was carried out under UV irradiation without the TiO2 foils. The minimum degradation under photolysis was 93.52 % at 30 oC after 20-minute UV-irradiation duration.
Fig. 7. The UV Spectra of furfural with and without Titanium foil at concentration of 250 mg.L-1 under 250W 100-minute UV-irradiation duration.
Fig. 8. The UV–VIS reflectance spectra of some samples at various degradation UV-irradiation durations for furfural (C= 250 mg.L-1) at pH 12 in the UV/TiO2/Pd system.
The effect of pH
As well known, the reactions involving ionic solutions are dependent on pH. The photocatalytic activity can be changed by the pH. Several sets of experiments were performed to determine the effect of initial pH
on the degradation of furfural. The furfural solutions were adjusted at a distinct pH by augment 1 M sulfuric acid and/or 1 M sodium hydroxide. They are also investigated at the pH of 1, 3, 7 and 12 (250 mg.L-1) under 250 W-UV irradiation in duration intervals of 20 min from 20 to 100 minutes.
After 100-minute UV-irradiation duration, the maximum degradation was 97.8% at pH 3 while the minimum was 95.8% at pH 12. The degradation values were as a parabolic function at various pH values. Also, while the irradiation duration was 70-75 min, the degradation values were independent of the pH values, as shown in Fig. 9.
Fig. 9. The effect of pH values on photocatalytic removal of furfural in the UV/TiO2/ Pd system
The effect of temperature
In the UV/TiO2/Pd system, the efficiency of decomposition was measured at 30 ºC and 40 ºC under UV-250W irradiation in duration intervals of 20 min from 20 to 100 minutes.
This efficiency for 100-minute UV-irradiation duration at optimum pH 3 was 96.70% and 98.5
% at 30ºC and 40 ºC, respectively. The results indicate that the maximum degradation (98.5%)
gives rise to the pH 3 and 40 ºC under UV irradiation.
The difference between the degradation values at 30 ºC and 40 ºC is decreased with increasing the UV-irradiation duration till 60 min, and then this difference is increased with increasing the UV-irradiation duration approximately, as shown in Fig. 10.
CONCLUSION
In this study, the UV/TiO2/Pd system in which the nanoparticles of palladium were doped into the titanium dioxide is proposed for degradation of furfural.
The experimental parameters of temperature, pH and UV irradiation duration may improve the photo catalytic process.
This process may be employed to reduce the furfural.
The results indicate that the maximum degradation occurs at a distinct pH and specific temperature under the UV irradiation.
The efficiency of furfural decomposition increases with increasing the UV-irradiation duration.
Also, while the irradiation duration is 70-75 min, the degradation values are independent of the pH values.
The difference between the degradation values at 30 ºC and 40 ºC is decreased with increasing the UV-irradiation duration till 60 min, and
then this difference is increased with increasing the UV-irradiation duration approximately.
ACKNOWLEDGEMENTS
We gratefully acknowledge the Nuclear Science and Technology Research Institute for financial and technical supports.